Preheating a heavy carbon steel weld assembly is a slow job by its nature: the heat has to travel through a lot of steel before the coldest point of the seam is at temperature. The trial described here does that job in a controlled, recorded cycle. Using the MYD-40KW air cooled induction heater, eight turns of flexible induction cable and a high-temperature insulation blanket, a welded carbon steel assembly of roughly 440 kg reached the required 177 °C (350 °F) preheat temperature in a single 28 minute heating cycle at 10-20 kHz, with a measured spread of only 4 K between the weld seam, the band edge and the inner ring.
The same equipment family is used for post weld heat treatment and stress relief work, so a fabricator that already owns an MYD generator can cover preheat, interpass control and post heating with the same power supply. The MYD induction PWHT machine page lists the published model range and the control and recording options.
Application overview
| Application | Induction preheating of a heavy carbon steel weld assembly before arc welding |
|---|---|
| Equipment | MYD-40KW air cooled induction heater |
| Frequency | 10-20 kHz |
| Heating time | 28 minutes (single power-on cycle to the preheat target) |
| Preheat target | 177 °C (350 °F) minimum at the weld seam |
| Base material | Magnetic carbon steel — outer shell ∅700 mm OD / ∅620 mm ID × 600 mm tall, inner ring ∅620 mm OD / ∅400 mm ID × 40 mm |
| Heated mass | Approximately 440 kg of steel |
| Heated band | 400 mm long, covered by a high-temperature insulation blanket |
| Heating coil | Flexible induction cable, 5 turns, arranged around the insulated band |
| Measurement | K-type thermocouples at the band edge, the weld seam and the inner ring, with curve recording |
| Average useful power | Approximately 18.5 kW over the 28 minute cycle |
| Result | 178 °C at the band edge, 182 °C at the seam, 179 °C on the inner ring, 4 K spread |
Why preheat a carbon steel weld at all
Carbon steel is a magnetic, readily heated material, and it is also the material most likely to suffer when a weld cools down too quickly. When the heat-affected zone next to the weld cools faster than its critical cooling rate, the austenite in that zone transforms into hard martensite instead of a softer structure. The result is a hardened, brittle band around the weld that resists subsequent forming and service loads. Where hydrogen is also present, as it is with most covered electrodes, that combination is the classic condition for hydrogen-assisted cracking.
Preheating addresses this by controlling how fast the weld metal and the surrounding parent metal cool. The joint is brought to a defined temperature before the arc is struck, so the heat capacity of the region is raised and the cooling rate through the critical range is reduced. The same preheat temperature also has to be maintained between passes, and both the minimum and the maximum allowed temperatures belong to the welding procedure specification.
It is worth being precise about what preheating is and is not. It is not a heat treatment, and it does not relieve residual stress. The temperature, the ramp rate and the hold time all come from the qualified welding procedure for the specific grade and thickness, not from the heating machine. The induction preheating welding machine page sets out the difference between preheat, interpass control, postheating and PWHT, and the selection data each of them requires.
Working principle
Alternating current in the flexible cable produces an alternating magnetic field around the assembly. That field induces eddy currents in the steel, and the resistance of those currents turns electrical energy into heat inside the metal itself. Because the heat is generated in the steel rather than transferred to it from a flame, the section is heated evenly from the inside out and the coating or insulation on the outside is not scorched.
Three practical details make the difference between a good preheat and a poor one. The cable turns must be spaced evenly so that no part of the band is over- or under-heated. The insulation blanket must cover the same band as the cable, because heat lost to the air is heat the generator has to make up. And the thermocouples have to be attached to clean metal at the positions the procedure requires, because a thermocouple only measures where it touches.

The air cooled induction heating system configuration used here has a specific practical advantage on site and in the workshop: the generator is cooled by forced air instead of a circulating water circuit, so there is no pump, chiller or cooling-water run to install around an installed vessel or a repair area. The heating cable is a separate item, and its cooling arrangement should be confirmed for the selected configuration.
Why 10-20 kHz for a heavy carbon steel assembly
Frequency selection decides where the heat lands. Skin depth grows as frequency falls, so a high-frequency band concentrates the induced current in a thin skin at the surface, while a medium-frequency band pushes the current further into the section. The section heated in this trial was a 40 mm wall shell together with a heavy inner ring, and the aim is to raise the temperature through the whole wall rather than only at the outer surface, because the weld seam and the root run are what have to be above the preheat temperature when the arc starts.
At 10-20 kHz the current penetrates deeply enough into the section to heat it through, while a 700 mm outside diameter still allows a practical cable arrangement with uniform turn spacing. Going lower in frequency would increase the effective heated mass and the power needed to hold the joint temperature, and going higher would concentrate the heat at the surface and lengthen the cycle considerably. The selected band also sits comfortably inside the published 2-36 kHz output range of the MYD series.
There is a second, often overlooked reason to stay in the medium band for a magnetic steel: the coupling changes as the material heats. The permeability of carbon steel falls as the temperature rises and collapses at the Curie point, which changes the impedance seen by the generator. Working inside a stable band with a controlled power program keeps the load matched and the heat predictable, rather than chasing a load that is changing under the coil.
The 28 minute heating cycle
Figure 2 shows the temperature recorded at three positions on the assembly. All three thermocouples follow the same ramp and reach the preheat requirement together at the end of the 28 minute cycle. The power is then switched off while the blanket is left in place, and the temperature equalises across the band: the hotter seam gives up heat to the cooler surrounding metal until the whole monitored area reads 180 °C. Arc welding started about 40 minutes after power on, with the joint still above the minimum preheat temperature.

The average ramp rate for this cycle is about 5.4 °C/min, calculated from 25 °C to 177 °C in 28 minutes. That sits at the low end of the published 5-400 °C/min heating-rate range of the MYD series, and that is deliberate: a large restrained assembly heated quickly develops thermal gradients that the joint cannot tolerate, so the long, slow ramp is a feature of the process rather than a limitation of the machine.
Temperature uniformity and the energy balance
Preheat is judged on the coldest point of the joint, not on the average. Figure 3 shows the axial temperature profile at the end of the cycle: a flat-topped plateau across the heated band, with measured values of 178 °C at the band edge, 182 °C at the weld seam and 179 °C on the inner ring, a spread of 4 K. The profile falls away quickly outside the band, which is why the band has to be sized so that the whole seam and the intended run-on length sit inside it.

The energy side of the cycle is simple to check. A heated steel mass of about 440 kg raised through 152 K needs roughly 31,000 kJ of sensible heat. Spread over 28 minutes that is an average useful power of approximately 18.5 kW, so a 40 kW machine is the right order of magnitude for an assembly of this size with good cable coupling and a properly insulated band. Heavier assemblies, longer bands, greater heat loss into surrounding structure or a colder ambient temperature all push the requirement up, and the figure has to be recalculated rather than scaled.
General guidance on selecting a generator, coil and heated band for a given diameter, wall thickness and cycle is available in the HLQ guide to induction preheating for welding steel, pipes and strips.
Preheat procedure
- Confirm the procedure. Take the preheat temperature, the permitted ramp rate, the interpass limits and the measurement positions from the qualified welding procedure specification. Do not take them from the equipment.
- Prepare the joint. Clean the surface where the thermocouples will be attached, square the joint and fit the groove. Check that the assembly is free of coating, paint or insulation in the heated band, since a coating in the band changes the coupling and the heat distribution.
- Install the thermocouples. Attach them to bare metal at the approved positions and identify every channel. The seam position and at least one band edge are the two points that decide whether the assembly is acceptable.
- Fit the blanket and the cable. Wrap the insulation over the band, then arrange the flexible cable turns at uniform spacing around the blanket. Secure the cable with non-metallic restraints so that no conductive loop is created around the assembly.
- Check the system. Verify the supply, the connections, the cooling airflow, the thermocouple readings and the recorder before starting. Confirm that the temperature trace is running; a missing chart cannot be reconstructed afterwards.
- Run the 28 minute cycle. Select the 10-20 kHz band, apply the programmed power and hold for 28 minutes, following the slow ramp that the assembly requires. Stop the heating at the end of the cycle rather than letting the controller overshoot the preheat requirement.
- Soak, verify and weld. Leave the blanket in place and allow the temperature to equalise across the band. Read the recorded temperatures at all monitored positions, confirm that the minimum is met everywhere, and start welding while the assembly is still above the preheat temperature.
Results and observations
| Preheat target | 177 °C (350 °F) minimum at the weld seam |
|---|---|
| Heating time | 28 minutes at 10-20 kHz with the MYD-40KW |
| Temperature survey at 28 min | 178 °C at the band edge, 182 °C at the seam, 179 °C on the inner ring |
| Temperature spread | 4 K across the monitored positions |
| Heated band | 400 mm, with the whole seam inside the preheat zone |
| Soak before welding | Power off at 28 min, temperature equalised under insulation, welding started at about 40 min |
| Surface condition | No scorching of coating or adjacent material |
| Operator factor | Low — the cycle is defined by the program and the recorded temperatures, not by flame technique |
| Main control point | Even cable turn spacing and blanket coverage; irregular spacing shows up as an uneven profile |
Two results are worth carrying into production planning. First, the heated band width, not the generator power, is usually the parameter that decides uniformity: with a 400 mm band the seam stayed within 4 K of the band edge, and a wider band would have required more power for the same cycle time. Second, the preheat does not end when the power stops, because the blanket holds the assembly above the minimum and lets the temperature equalise; that soak time can be used to call the welding procedure, but it should be counted separately from the 28 minute heating cycle.
Advantages over oxy-fuel torch preheating
- No flame at the joint. The assembly is heated by induction, so there is no burner, no ignition source and no hot gas plume next to coated pipe, insulation or a live hydrocarbon line.
- Measured, not judged. The temperature is recorded at defined positions instead of being estimated from the colour of the metal, so every assembly in a series receives the same treatment.
- Heat in the steel, not on it. Because the energy is deposited inside the section, the outer coating and insulation are not scorched and the joint is not heated unevenly from one side.
- A defined band. Only the preheat zone is heated. The rest of the assembly stays close to ambient, which matters on large components with sensitive coatings.
- No cooling-water circuit on site. The air cooled generator removes the pumps, chillers and water runs that a water cooled unit would need, which simplifies field work and repair work on installed piping.
- Repeatable cycles. Once the program is qualified for an assembly, every following one is heated to the same condition with a recorded curve for the weld record.
For pipeline, pressure vessel and structural applications the induction preheating for welding application pages cover the coil options and the accessories, including the flexible cable and the insulation blankets, and the PWHT flexible cable coil page describes the working inductor used for this type of heating.
Frequently asked questions
How long does induction preheating take for a carbon steel weld assembly?
In this trial the assembly reached the 177 °C (350 °F) preheat requirement in 28 minutes of induction power-on at 10-20 kHz with the MYD-40KW air cooled induction heater. The 28 minute figure is the heating time to the target only. The assembly was then held under insulation so the temperature equalised across the band, and arc welding started about 40 minutes after power on.
Why is 10-20 kHz used for preheating a heavy carbon steel assembly?
Skin depth increases as frequency decreases, and the heated mass here was a 40 mm wall shell together with a heavy inner ring rather than a thin sheet. At 10-20 kHz the induced current penetrates far enough into the section to raise the temperature through the wall instead of only heating the outer skin, which is what allows the weld seam to reach the preheat temperature at the same time as the surrounding metal. The band also sits comfortably inside the published 2-36 kHz output range of the MYD series.
What preheat temperature is required for welding carbon steel?
The requirement comes from the welding procedure specification and the governing code, not from the heating equipment. It depends on the carbon equivalent of the grade, the wall thickness, the hydrogen level of the consumable and the restraint of the joint. The 177 °C (350 °F) figure used here is the value specified for the tested assembly and must not be transferred to another grade or thickness without qualification.
How is the heated band width and the temperature uniformity controlled?
The heated band is set by the cable arrangement, and the blanket covers the same area so that heat is not lost before it reaches the metal. In this trial a 400 mm band with eight cable turns produced a measured spread of 4 K between the band edge, the weld seam and the inner ring, with a minimum of 178 °C across the monitored points at the end of the cycle. Turn spacing, insulation coverage and the number and position of the thermocouples are the three controls that determine uniformity.
How much electrical power is needed to preheat a large weld assembly?
For the tested assembly the heated steel mass was about 440 kg and the temperature rise was 152 K, which corresponds to roughly 31,000 kJ of sensible heat. Spread over a 28 minute cycle this is an average useful power of about 18.5 kW, so the 40 kW MYD-40KW class is appropriate for an assembly of this size with good cable coupling and insulation. Larger diameters, thicker walls, longer bands or greater heat loss into surrounding structure require a recalculation and usually a larger model.
Why does the assembly need a soak period after the heating cycle?
A large assembly does not heat uniformly in one pass. The metal closest to the cable runs hot while the inner ring and the band edges lag behind, so the measured points can differ by several degrees even inside the target band. Holding the assembly under insulation after power off lets conduction even out the difference, and the temperature survey confirms that the whole monitored band is at or above the minimum before welding starts.
What are the advantages of induction preheating compared with oxy-fuel torch preheating?
Induction heating puts the heat inside the steel instead of delivering it from a flame, so there is no burner, no combustion gases and no local scorching of coating or insulation. The temperature is measured and recorded rather than judged by the colour of the metal, so every assembly receives the same energy. The heat is applied in a defined band, the unit can be moved to the joint instead of the joint to a furnace, and an air cooled generator avoids a cooling-water circuit on site.