Induction Brazing of T-Shaped Copper Assemblies
Simultaneous Induction Brazing of T-Shaped Copper Assemblies with the HLQ DWS-30
Joining a T-shaped copper assembly normally means lighting a torch three times and waiting for three separate joints to reach brazing temperature one after the other. The trial described below does it the other way round. Using the DWS-30 Handheld Induction Heater, a custom multi-zone coil and preformed copper-phosphorus-silver filler rings, all three joints of a ∅42 mm × 0.6 mm copper tee assembly reached the filler working range inside a single heating cycle of 45 seconds at 40-60 kHz.
The result matters most for HVAC and refrigeration lines, where a T-junction on a large thin-wall copper line is one of the slowest and least repeatable joints on the assembly line. The same principle behind this work is described in more detail in our guide to optimizing HVAC brazing with induction heating.
Application overview
| Application | Simultaneous induction brazing of three joints on a T-shaped copper assembly |
|---|---|
| Industry | HVAC and refrigeration manufacturing |
| Equipment | DWS-30 Handheld Induction Heater |
| Frequency | 40-60 kHz |
| Heating time | 45 s (single power-on cycle for all three joints) |
| Base material | Copper tubing and copper fittings |
| Copper tubing diameter | ∅42 mm |
| Copper tubing thickness | 0.6 mm wall |
| Filler metal | Preformed Cu-P-Ag (copper-phosphorus-silver) rings |
| Coil | Custom three-zone induction coil matched to the joint layout |
| Joints per cycle | 3 (two straight-run couplings + one branch socket) |
Working principle
Alternating current in the coil produces an alternating magnetic field. That field induces eddy currents in the copper, and the electrical resistance of those currents generates heat directly inside the metal — no flame, no hot air, no contact between the tool and the part.
For simultaneous brazing the whole problem is heat distribution. If the coil only wraps around one socket, the other two joints depend on heat travelling along the tube, which is slow and uneven: the first joint overheats while the last one is still cold. The solution used here is a coil with three shaped heating zones — one around each coupling and one around the branch socket — so that every joint receives a comparable share of the electromagnetic energy at the same time. This is the same design logic that HLQ applies when it engineers custom induction brazing coils for a customer’s specific joint geometry.

Figure 1 shows the three heating zones, the eddy current paths in the tube wall and the position of the preformed filler rings. The same arrangement is used across many joint families; our existing three-joint copper tee induction brazing application describes the smaller-diameter version of the same concept.
Why 40-60 kHz suits a ∅42 mm × 0.6 mm tube
Frequency selection is the single most consequential decision in this application, and for thin-wall large-diameter copper it points in a clear direction.
Skin depth is proportional to the square root of the resistivity divided by the product of frequency and permeability. Copper is a good conductor, so at high frequencies the induced current is confined to a very thin outer layer of the tube. On a ∅42 mm tube with a 0.6 mm wall, a high-frequency band heats the outer skin of the tube and leaves the inner surface of the wall comparatively cold, so the joint has to run longer to bring the full section up to temperature.
At 40-60 kHz the current penetrates deeply enough to raise the temperature through the whole 0.6 mm section, while the 42 mm diameter still permits a compact coil with a good coupling distance. The heating is therefore closer to a true volumetric heating of the wall, which is what allows three joints to come up together in one short cycle. Moving lower still would increase the effective heated mass and the power required to hold the joint temperature.
The handheld induction brazing heater used for the trial is the DWS-30 unit, rated at 30 kW maximum input power with a remote heating head of approximately 3.1 kg, which keeps the operator close to the joint and the tool usable in confined installation work as well as on a production line. A lower-power alternative is available as a portable induction brazing heater for smaller tube sizes.
Key process parameters
| Parameter | Setting | Why it matters |
|---|---|---|
| Equipment | DWS-30 Handheld Induction Heater | 30 kW class generator with remote heating head |
| Frequency | 40-60 kHz | Deep penetration into a 0.6 mm wall at ∅42 mm diameter |
| Heating time | 45 s | Single power-on cycle covering all three joints |
| Tube size | ∅42 mm × 0.6 mm wall | Defines heated mass, coupling and coil clearance |
| Coil | Custom three-zone design | Even energy distribution across the three sockets |
| Filler | Cu-P-Ag preformed rings | Controlled filler quantity, no added flux on clean copper |
| Joint clearance | 0.02-0.05 mm | Capillary draw of the filler through the socket |
How the filler reaches the joint
Induction heating supplies the energy, but joint quality is decided by the filler behaviour. Once the socket surfaces reach the liquidus temperature of the Cu-P-Ag ring, the filler wets the prepared copper and is pulled into the clearance by capillary action. The 0.6 mm wall is worth protecting here: because only the filler melts and the tube never does, there is no wall thinning, no erosion and no distortion of the joint — which flame brazing can cause on thin-wall copper when the tip lingers.

The preformed ring is the reason the process is so repeatable. A ring of known diameter and cross-section delivers exactly the filler volume the joint needs and sits in a defined position in the socket, so the joint does not depend on the operator’s judgement of how much wire to feed in.
Heating cycle and temperature balance
Temperature is the acceptance criterion for a brazed joint, and the three sockets of this assembly do not heat identically. The branch socket carries more copper mass than a straight-run coupling because the tube wall and the tee body overlap there, so it reaches the filler working range slightly later than the two straight joints unless the coil is matched to compensate.

The 45 s power-on time shown in Figure 3 is the point at which all three joints had entered the 600-650 °C working range of the filler, after which the power was switched off and the assembly was allowed to solidify. Because the induction heating stops at the end of the cycle, there is no continuing heat input to the joint, and the filler freezes almost immediately once the power is removed.
Brazing procedure
- Prepare the parts. Cut the copper tube square, deburr the end and clean the mating surfaces. On a 0.6 mm wall, a light draw filing of the tube end is usually enough to make the tube enter the socket without force, which prevents the tube from being pinched or ovalised.
- Dry fit and check the clearance. Assemble the tee and both couplings by hand and confirm a uniform 0.02-0.05 mm gap between tube and socket. Excess clearance starves the joint of filler; too little clearance prevents the filler from entering at all.
- Place the filler. Position one correctly sized Cu-P-Ag ring at each of the three sockets. Do not add extra flux on clean copper-to-copper surfaces; the Cu-P family is effectively self-fluxing and surplus flux is the main cause of residue inside the assembly.
- Position the coil and load the fixture. Set the three heating zones over the three joints with a consistent gap from the copper, and locate the assembly in a fixture so that the coil-to-joint relationship repeats from one cycle to the next. Repeatability of coil position is what makes the 45 s cycle reproducible.
- Heat. Select the 40-60 kHz band, apply power and hold for 45 s, watching the filler rather than the colour of the copper. The filler should visibly flow and settle into the socket.
- Cool and inspect. Switch off, hold the assembly in the fixture until the filler has solidified, then check all three joints for wetting and fillet continuity and run the specified leak test.
Results and observations
| Joints brazed per cycle | 3 (all joints completed in one 45 s heating cycle) |
|---|---|
| Heating time | 45 s at 40-60 kHz |
| Tube | ∅42 mm outside diameter, 0.6 mm wall, no distortion after cooling |
| Filler | Cu-P-Ag rings, no additional flux required on clean copper |
| Surface quality | Clean joint area, minimal residue, no scorching of adjacent tube |
| Operator factor | Low — the cycle is governed by the timer and the coil position, not by torch technique |
| Balance requirement | Branch socket lags the straight joints slightly and needs coil compensation |
Two observations are worth carrying forward into production. First, the branch socket of a tee runs behind the straight-run couplings because of the extra copper mass where the tube wall meets the tee body; a coil designed for straight couplings alone will not balance the three zones. Second, the station cycle is longer than the 45 s of induction heating — loading, positioning, cooling and unloading must be timed separately if a production rate is being quoted.
Advantages over torch brazing
The business case for moving this joint to induction is mostly about control rather than speed, although the speed is welcome.
- No open flame. On an HVAC line the joint is often close to insulation, refrigerant charge and painted sheet metal. Removing the torch removes the fire risk and the risk of burning or discolouring adjacent parts.
- Repeatable results. The cycle ends on a timer, so every joint receives the same energy instead of depending on the operator’s torch technique and judgement of colour.
- Clean joints. With a preformed ring and no added flux on copper, the residue that normally has to be cleaned out of the line afterwards is largely avoided.
- The base metal is protected. On a 0.6 mm wall, controlling where the heat goes prevents the erosion and thinning that a torch tip left too long in one spot causes.
- Power and water are managed by the machine. The generator handles power delivery and the water-cooled coil handles coil temperature, so the process is less sensitive to operator skill and ambient conditions.
If you are comparing machines for this kind of work, our induction brazing machine range and the dedicated induction brazing application pages cover the equipment and coil options in more detail.
Frequently asked questions
Can three copper joints be brazed at the same time?
Yes. With a purpose-built three-zone coil and a matched power setting, the DWS-30 handheld induction heater brought the two straight-run couplings and the branch socket of this T-shaped assembly into the filler working range inside a single 45 s power-on cycle at 40-60 kHz. The key is coil geometry: each socket has to receive comparable energy rather than relying on heat conduction from one hot point.
Why use 40-60 kHz for a ∅42 mm diameter copper tube with a 0.6 mm wall?
Skin depth grows as frequency falls. At 40-60 kHz the induced current penetrates far enough into the 0.6 mm wall to heat the tube through its full section, while the 42 mm diameter still allows a reasonably short, efficient coil. A high-frequency band would concentrate the heat on the outer surface of a thin, large-diameter tube and lengthen the cycle.
How long does the brazing cycle take?
The recorded heating time is 45 s of induction power-on for the complete three-joint assembly. The 45 s figure is induction heating only; loading, positioning, cooling and unloading are separate steps in the station cycle and should be timed independently for production planning.
Which filler metal and flux are used?
Preformed copper-phosphorus-silver (Cu-P-Ag) rings sized to the socket clearance. On clean copper-to-copper surfaces the Cu-P family is effectively self-fluxing, so no additional flux was required for this trial. Confirm the flux requirement against the filler supplier for the specific material combination and service condition.
Is the base copper melted during induction brazing?
No. Brazing does not melt the base metal. Only the filler metal is taken to its liquidus temperature, where it wets the prepared surfaces and is drawn into the 0.02-0.05 mm joint clearance by capillary action. The tube and fitting stay well below their melting point, which protects the thin 0.6 mm wall from erosion and distortion.
What are the main advantages of induction brazing over torch brazing?
There is no open flame, so the risk of fire and of burning adjacent insulation or refrigerant lines is removed. Heating is repeatable, the operator does not control temperature by eye, cycle time is predictable, and the joint area stays clean because filler and flux residue are confined to a small zone.