Induction Melting Brass

Induction Melting Brass with Zinc-Loss Control

Quick Answer

Induction melting brass melts the copper-zinc charge with eddy currents from a water-cooled coil fed by a medium-frequency IGBT power supply. The electromagnetic field also stirs the bath, which keeps the zinc evenly distributed.

Brass melts at about 885–955 °C, depending on grade. Zinc boils at 907 °C, so zinc loss is the main process risk. To control it:

  • Hold the melt at 950–1,020 °C, and never above 1,050 °C.
  • Keep holding time short.
  • Add zinc last.
  • Keep a flux cover on the melt.
  • Run fume extraction throughout the heat.
  • Use a silica lining (SiO₂ ≥ 97%).
Melting brass in an induction coil
Brass melting inside an induction coil.

What is Induction Melting Brass?

Induction melting brass is the melting of copper-zinc alloys in a coreless induction furnace. A medium-frequency generator, compensating capacitors and the furnace body make up the system. An infrared temperature sensor and controller can be added.

The furnace can be a tilting, push-up or stationary type. Tilting furnaces are tilted manually, electrically or hydraulically. Stirring helps flux and oxides float to the surface, which gives cleaner castings.

For pure copper, see induction melting copper.

Brass induction melting bath
Molten bath in an induction furnace.

Key Applications

Brass induction melting selection chart: power and frequency by application, silica lining data and DW-MF power supply models
Application and selection chart: power and frequency by application, silica lining data and DW-MF models.
Application Alloys Capacity Key requirement
Brass valve and fitting production C36000, C28000, C37700 200–1,000 kg Zinc-loss control, fast cycle, consistent chemistry
Small brass foundry C26000, C36000 100–300 kg Zinc-loss control; fume extraction
Medium brass / bronze foundry C28000, C90500 300–1,000 kg Hydraulic tilt; PLC control; batch production
Laboratory and small casting All copper alloys 5–100 kg Flexible alloy switching
Brass scrap recycling Sorted brass scrap By project Sorting and drying; zinc recovery by vacuum distillation

To recover zinc and copper separately from brass scrap, see the copper zinc separation furnace.

Induction melting copper and brass in a tilting furnace
Copper-alloy charge melting in a tilting induction furnace.

Suitable Materials

Grade Name Melting range Density Recommended lining Special handling
C26000 Cartridge brass 70/30 915–955 °C 8.53 kg/dm³ Silica (SiO₂ ≥ 97%) Zinc fuming; fume extraction required
C28000 Muntz metal 60/40 900–940 °C 8.39 kg/dm³ Silica Higher zinc loss; temperature control critical
C36000 Free-cutting brass 885–900 °C 8.50 kg/dm³ Silica or alumina-silica Lead content; ventilation required
Brass returns and scrap Sorted by alloy Varies Bulk 2–5 kg/dm³ Match to the dominant alloy Pre-sort, pre-dry, manage dross

The same furnaces also melt copper, bronze, silver, gold, aluminum and steel, with the lining and frequency chosen for each metal.

Working Principle

How induction melting brass works: DW-MF power supply, capacitor bank, coil, silica lining, flux cover, stirring and zinc-loss limits
Principle diagram: medium-frequency supply, resonant circuit, coil, silica lining, brass charge and stirring.
  1. Power: The IGBT inverter converts 3-phase mains into 1–20 kHz current.
  2. Resonance: The coil and compensating capacitors form a resonant circuit.
  3. Heating: The coil’s alternating field induces eddy currents in the brass charge, and Joule heating melts it.
  4. Stirring: Electromagnetic stirring distributes the zinc evenly, so it does not segregate.
  5. Zinc control: Zinc boils at 907 °C, so temperature and holding time decide how much zinc is lost.

Background: how an induction heater works.

Silica lining for brass

Item HLQ data
Lining type Silica (acid), SiO₂ ≥ 97%
Sintering temperature 1,050–1,100 °C
Expected life 200–400 heats
Primary failure mode Thermal cycling erosion
Alloy switching Do not melt pure copper in a lining used for brass; zinc in the lining can contaminate the copper

Technical Specifications

Parameter DW-MF medium-frequency melting system
Power range 15–160 kW maximum input (DW-MF-15 to DW-MF-160)
Frequency 1–20 kHz; typical 4, 8, 11, 15 or 20 kHz depending on application
Supply 3 × 380 V ±20%, 50 or 60 Hz
Duty cycle 100%, 24-hour operation
Melting capacity range 3–500 kg
Melt time About 50–60 min from a cold furnace; 20–30 min in a hot furnace
System MF generator, compensating capacitors, melting furnace; optional infrared sensor and temperature controller
Furnace types Tilting (manual, electrical, hydraulic), push-up, stationary
Brass melt temperature 950–1,020 °C recommended; never above 1,050 °C
Lining Silica, SiO₂ ≥ 97%
Small tilting brass melting furnace with medium frequency induction power supplies
Small manual-tilting furnace with medium-frequency power supplies.

Recommended Model Selection

Application Alloys Capacity Power Frequency Key feature
Laboratory / small casting All copper alloys 5–100 kg 15–75 kW 2,000–8,000 Hz Compact; tilt pour
Small brass foundry C26000, C36000 100–300 kg 75–200 kW 1,000–2,500 Hz Zinc-loss control; fume extraction
Medium brass / bronze foundry C28000, C90500 300–1,000 kg 200–700 kW 500–1,500 Hz Hydraulic tilt; PLC control

DW-MF power supplies

Model DW-MF-15 DW-MF-25 DW-MF-35 DW-MF-45 DW-MF-70 DW-MF-90 DW-MF-110 DW-MF-160
Max input power 15 kW 25 kW 35 kW 45 kW 70 kW 90 kW 110 kW 160 kW
Weight 50 kg 50 kg 65 kg 70 kg 80 kg 94 kg 114 kg 145 kg

Details: medium frequency induction melting furnace for copper and brass. For 100–1,000 kg brass and bronze, see the induction copper and brass melter.

Process Workflow

Induction brass melting process flow with flux cover, zinc added last and 950–1,020 °C temperature control
Process flow chart: twelve steps with brass zinc-loss controls.
Step Action Control point
1 Inspect the lining and cooling water; start fume extraction Extraction running throughout the heat
2 Preheat the lining or crucible Avoid thermal shock
3 Sort the charge by alloy, weigh it and pre-dry the scrap No wet scrap in a hot furnace
4 Load dense material first —
5 Raise power gradually —
6 Add the remaining charge as the first batch melts —
7 Apply a flux cover (charcoal or copper flux) Keep the cover on during the heat
8 Add zinc as the last element Limits zinc loss
9 Hold at 950–1,020 °C Never above 1,050 °C; short holding
10 Skim the dross Clean surface before pouring
11 Check the temperature and take a sample Cu-Zn composition
12 Tilt and pour into a ladle or moulds —

Workshop layout

Brass melting workshop layout with DW-MF power supply, capacitor box, cooling, tilting furnace, fume extraction, thermocouple, dross bin and pouring area
Layout diagram (schematic, not to scale) of a brass melting workshop.

Common Problems and Solutions

Problem Likely cause Solution
Zinc fuming Temperature above 1,050 °C; long holding Reduce to 950–1,000 °C; minimize holding; add zinc last; check fume extraction
Hydrogen porosity in castings Wet or oily scrap; damp flux Pre-dry all scrap and flux; purge with dry argon
Rapid lining erosion Wrong lining chemistry, overheating, poor sintering, thermal shock Use a silica lining; follow the sintering protocol; preheat the charge
Alloy out of specification Charge error, volatile zinc loss, contaminated scrap Recalculate the charge; add volatile elements last; use certified scrap
Inconsistent chemistry between heats Variable scrap, manual addition errors, sampling Sort scrap; standardize sampling
Pure copper contaminated after brass Zinc absorbed in the lining Use a dedicated lining or furnace for each alloy family
Furnace fails to start Coil insulation fault, water flow alarm, IGBT or capacitor fault Check coil insulation (> 1 MΩ), water flow, IGBT and capacitor fuses

Engineering Selection Guide

Factor What to confirm Recommendation
Brass grade C26000, C28000, C36000 or other Sets the melt temperature and ventilation needs (lead in C36000)
Throughput Net kg/h with a 70% utilization factor Sets furnace capacity and power
Charge form Ingot, returns or scrap Scrap must be sorted and dried
Lining Dedicated to brass or shared with other alloys Silica; keep a separate lining for pure copper
Fume extraction Hood above the furnace Required for zinc and lead fumes
Pouring Manual, electrical or hydraulic tilt Hydraulic for larger batches; see the hydraulic tilting copper melting furnace
Scale-up Future capacity The 5–5000 kg copper melting induction furnace range covers brass up to industrial size

Advantages and Limitations

Advantages Limitations
Electromagnetic stirring distributes zinc evenly Zinc fuming needs dedicated fume extraction
Precise power control helps hold 950–1,020 °C The temperature window must be held to limit zinc loss
Stirring helps flux and oxides float, for cleaner castings A lining used for brass should not be used for pure copper
About 20–30 min per melt in a hot furnace Lead-bearing brass needs ventilation
One furnace also melts copper, bronze, silver, gold and aluminum Cooling water is required

Why Choose HLQ?

Strength What it means
DW-MF series 15–160 kW, 1–20 kHz, 100% duty cycle
Brass process practice Temperature window, zinc added last, flux cover, fume extraction
Silica linings Selected and sintered for brass
Furnace options Tilting (manual, electrical, hydraulic), push-up or stationary
Scale-up path Copper-alloy furnaces from 5 kg to 5,000 kg
Zinc recovery Copper-zinc vacuum separation furnaces for brass scrap

10 Core FAQs

1. At what temperature does brass melt?

C26000 at 915–955 °C, C28000 at 900–940 °C and C36000 at 885–900 °C.

2. What temperature should the melt be held at?

About 950–1,020 °C for most brass alloys, and never above 1,050 °C.

3. Why does brass lose zinc during melting?

Zinc boils at 907 °C, so it fumes at brass melting temperatures. Overheating and long holding make the loss worse.

4. How do I reduce zinc loss?

Control the temperature, minimize holding time, add zinc last, keep a flux cover and run fume extraction.

5. Which lining should I use?

Silica with SiO₂ ≥ 97%, sintered at 1,050–1,100 °C. Expect about 200–400 heats.

6. Can I melt pure copper after brass in the same furnace?

Not in the same lining. Zinc absorbed in the lining can contaminate the copper, so use a dedicated lining or crucible.

7. Which power supply is used?

DW-MF medium-frequency IGBT supplies, 15–160 kW at 1–20 kHz, 3 × 380 V, 100% duty cycle.

8. How long does one melt take?

About 50–60 minutes from a cold furnace and 20–30 minutes in a hot furnace.

9. What power does a brass foundry need?

75–200 kW at 1–2.5 kHz for 100–300 kg, and 200–700 kW at 0.5–1.5 kHz for 300–1,000 kg.

10. Is lead-bearing brass a problem?

Free-cutting brass C36000 contains lead, so ventilation is required.