Induction Annealing of Thread Ring Gage Blocks
Annealing Thread Ring Gauge Blocks with a DW-UHF-10KW Induction Heater at 258 kHz
Objective:
To selectively and uniformly anneal two sections of a thread ring gage block from the hole to the outside surface from a hardness of Rc 59-61 to Rc 45. The gage blocks are made from O6 steel and range in size from 1″ to 8 1/2″ in diameter and run from 1/4″ to 1″ thick. Production is currently performed using a flame torch at an approximate rate of 250 to 300 of each part per month. Process goals include possible automation, production rate increase, and elimination of stress cracking resulting from flame heating.
End Product:
| Item | Specification |
|---|---|
| End product | Gauge Blocks |
| Part type | Thread ring gage block |
| Heat-treated feature | Two sections, from the hole to the outside surface |
Equipment:
| Item | Specification |
|---|---|
| Power supply | DW-UHF-10KW Induction Heater |
| Remote heat station | Three (3) busses and two (2) capacitors with a total capacitance of 0.66 µF |
| Induction coil | Flat front-load coil, designed and developed specifically for this application |

The published specification of the DW-UHF-10KW induction heater is reproduced below as published by the manufacturer.
| Technical parameter | Specification |
|---|---|
| Manufacturer | HLQ Induction Equipment Co., Ltd. |
| Model | DW-UHF-10KW |
| Heating technology | Ultra-high-frequency induction heating |
| Rated output power | 10 kW |
| Available frequency options | 50–300 kHz or 100–500 kHz |
| Input voltage | 380 V ±10% |
| Input power supply | Three-phase AC |
| Input frequency | 50/60 Hz |
| Input current | 3–15 A (published specification; to be confirmed) |
| Power electronics | IGBT inverter technology |
| Operating modes | Constant current / constant power |
| Rated duty cycle | 100% (subject to specified cooling conditions) |
| Main unit dimensions | 570 × 260 × 500 mm |
| Main unit weight | Approximately 30 kg |
| Heating method | Electromagnetic induction |
| Temperature control | Application-dependent; optional monitoring and control configuration |
| Installation | Industrial workshop / production line |
| Automation | Customized integration available |
Materials:
| Item | Specification |
|---|---|
| Material | Gage blocks made from O6 oil-hardened steel |
| Outside diameter | 1″ to 8 1/2″ |
| Thickness | 1/4″ to 1″ |
| Starting hardness | Rc 59-61 |
| Finished hardness in the annealed zones | Rc 45 |
| Condition outside the annealed zones | Unchanged; the body, bore and internal thread keep their original condition |
The material and the part size drive every other parameter in the process, because O6 steel is a through-hardening tool steel that responds quickly and evenly to a controlled high-frequency thermal cycle, and because the two heat-treated zones must be brought from Rc 59-61 to Rc 45 without the rest of the block following them.
| Part characteristic | Published value | Why it matters to the process |
|---|---|---|
| Material | O6 oil-hardened steel | Through-hardening tool steel; the heat-treated zones must be softened selectively without affecting the rest of the block |
| Outside diameter | 1″ to 8 1/2″ | Sets the coil footprint and the power needed to bring the full zone to temperature |
| Thickness | 1/4″ to 1″ | Sets the coupling gap and therefore how quickly the zone heats through |
| Heat-treated region | Two sections, from the hole to the outside surface | The selective requirement; the bore, the thread and the remaining body are not annealed |
Temperature:
| Item | Specification |
|---|---|
| Annealing temperature | 1300 °F (704 °C) |
| Hold requirement | Held until the zone is uniformly through heat from the hole out to the outside surface |
| Unheated region | The bore, the internal thread and the block body do not reach the anneal temperature |
The temperature is held long enough for the zone to be uniformly through heat, not just hot at the surface nearest the coil. That distinction is the whole reason the induction route solved this job: a flame torch applied from one side could raise the outer face of the zone without bringing the material near the hole to the same condition, which is what produced the uneven results and the cracking.
Frequency:
| Item | Specification |
|---|---|
| Operating frequency | 258 kHz |
| Machine frequency options | 50–300 kHz or 100–500 kHz |
| Power on time | 15 seconds |
| Annealed band | Two zones, from the hole to the outside surface |
| Cycle time | 7.5 to 12 seconds depending on part size |
| Production rate | 250 to 300 parts per month |
258 kHz sits inside the published DW-UHF-10KW frequency options of 50–300 kHz or 100–500 kHz, and it is the band that produces the shallow, tightly controlled surface heating this job needs on a lightly gauged part.
The published catalogue table for the ultra-high-frequency band, which places the DW-UHF-10KW in context against the rest of the range, is reproduced below exactly as published.
| Model | Rated power | Input current | Oscillation frequency | Input supply | Duty cycle |
|---|---|---|---|---|---|
| DW-UHF-3.2KW | 3.2 kW | 13 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-4.5KW | 4.5 kW | 20 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-045T | 4.5 kW | 20 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-045L | 4.5 kW | 20 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-6.0KW | 6.0 kW | 28 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-06A | 6.0 kW | 28 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-6KW-B | 6.0 kW | 28 A | 1.1–2.0 MHz | Single-phase 220 V ±10% | 100% |
| DW-UHF-10KW | 10 kW | 15 A | 100–500 kHz | 3 × 380 V ±10% | 100% |
| DW-UHF-20KW | 20 kW | 30 A | 50–250 kHz | 3 × 380 V ±10% | 100% |
| DW-UHF-30KW | 30 kW | 45 A | 50–200 kHz | 3 × 380 V ±10% | 100% |
| DW-UHF-40KW | 40 kW | 60 A | 50–200 kHz | 3 × 380 V ±10% | 100% |
| DW-UHF-60KW | 60 kW | 90 A | 50–150 kHz | 3 × 380 V ±10% | 100% |
Principle

The block is placed in a flat front-load coil and the alternating current at 258 kHz induces eddy currents in the two zones that sit inside the coil windows. Those currents heat the steel directly, from within the material, with no flame anywhere near the part. The heat is confined to the two zones, so the bore, the internal thread and the body of the block between them stay at their original Rc 59-61 condition while the zones are brought to 1300 °F.
The remote heat station carries three busses and two capacitors with a total capacitance of 0.66 µF, and this is what makes the coupling consistent from part to part. Because the same coil geometry and the same electrical configuration are used on every block, the two zones reach the anneal temperature together rather than one running ahead of the other.
Uniformity of heating is the mechanism that eliminates the stress cracking. A flame torch heats from the outside in, so the material near the bore is always cooler than the material at the outside surface during the ramp, and the temperature gradient across the zone sets up stresses that crack the hardened steel. Induction heating with a purpose-designed coil applies the energy evenly over the full width of the zone, so the gradient that causes cracking is not created.
For comparison, HLQ’s published reference application for induction annealing of bolt shafts uses the same family of machine and the same remote workhead architecture, which confirms that the workhead and the coil are the two components that decide the outcome in this class of heat treatment. The wider induction heating coil range covers the standard configurations for comparison against this custom front-load design.
Testing:
The DW-UHF-10KW Induction Heater was utilized to achieve the following objectives:
- Production time is reduced to less than 12 seconds per part due to a unique coil, designed specifically for heating both zones simultaneously.
- Stress cracking, previously experienced with flame annealing, is eliminated through uniform heating attained from the uniquely designed coil.
Automation is now possible, because the two annealing zones can be heated simultaneously in a front load coil.


The eight controlled stages that take a block from inspection to a verified hardness reading are set out below. Stages 5 and 6 are where the quality of the result is decided, because they are the stages in which the zone must become uniformly through temperature from the hole out to the outside surface.
- Part inspection. The block is checked for size and condition before loading, and the size within the 1″ to 8 1/2″ range is confirmed.
- Surface preparation. The block is degreased, and scale and oxide are removed from the two zones that are to be annealed.
- Coil loading. The block is slid into the front-load coil, with the two zones aligned to the coil windows.
- Power ramp. The DW-UHF-10KW output is raised, and current is induced in the two zones only.
- Ramp to 1300 °F. Both zones reach 704 °C simultaneously, because the coil couples them together.
- Soak and equalize. The heat is held so that the zone is uniformly through temperature, from the hole out to the outside surface.
- Controlled cooling. The coil is de-energised and the block is allowed to cool without distortion.
- Hardness verification. A Rockwell check confirms Rc 45 in both annealed zones.
The common problems specific to this application, and the process control that answers each one, are set out below.
| Problem | Cause | Solution |
|---|---|---|
| Stress cracking in the annealed zone | Non-uniform heating, and the temperature gradient that a flame torch creates across the zone | Uniform heating from the uniquely designed front-load coil, which eliminates the cracking previously experienced with flame annealing |
| Zone annealed at the outer face but not near the hole | Heat applied from one side only | Soak and equalize stage, holding the heat until the zone is uniformly through temperature from the hole to the outside surface |
| The two zones reaching temperature at different times | Poor coil symmetry or an inconsistent power history | A coil designed to heat both zones simultaneously, with constant current or constant power operation on the machine |
| Cycle time too long to reach the required rate | Heating one zone at a time | Both zones heated simultaneously in the front load coil, which brings the cycle to 7.5 to 12 seconds |
| The bore, thread or block body also softening | Heat spreading beyond the coil windows | Heat is applied only inside the coil windows, so the rest of the block never sees the anneal temperature |
| Oxide or scale forming on the zone | Surface contamination left on the part before heating | Degreasing and the removal of scale and oxide from the two zones during surface preparation |
| Part distortion after cooling | Uncontrolled cooling or uneven thermal contraction | Controlled cooling stage with the coil de-energised and the part allowed to cool without distortion |
| Inconsistent results between operators | Manual technique variation | A repeatable preset heating cycle on the machine, with the same coil geometry and workhead configuration on every part |
Benefits:
The final cycle time through induction heating ranged from 7.5 to 12 seconds, depending on the part size, which satisfies the present production rate of 250 to 300 parts per month.
| Benefit | Published outcome |
|---|---|
| Cycle time | 7.5 to 12 seconds per part, depending on part size |
| Production rate | 250 to 300 parts per month, satisfying the existing requirement |
| Stress cracking | Eliminated through uniform heating |
| Production time per part | Reduced to less than 12 seconds |
| Automation | Now possible, since both zones are heated simultaneously in a front load coil |
| Heat treatment quality | Two zones annealed uniformly from the hole to the outside surface, Rc 59-61 to Rc 45 |
| Operator involvement | Hands-free heating that involves no operator skill for manufacturing |
Summary
The DW-UHF-10KW Induction Heater at 258 kHz, with its remote heat station of three busses and two capacitors totalling 0.66 µF and a flat front-load coil designed for this application, anneals the two heat-treated sections of a thread ring gage block from the hole out to the outside surface, taking the hardness from Rc 59-61 to Rc 45 at 1300 °F (704 °C).
The single most important engineering decision in the application is that both zones are heated at the same time by one coil. It is what brings the cycle to 7.5 to 12 seconds per part, it is what removes the temperature gradient that cracked the parts when they were flame annealed, and it is what makes the cell suitable for automatic loading and unloading.
| Parameter | Value |
|---|---|
| Equipment | DW-UHF-10KW Induction Heater |
| Remote heat station | Three busses and two capacitors, total capacitance 0.66 µF |
| Coil | Flat front-load coil, designed to heat both zones simultaneously |
| Frequency | 258 kHz |
| Temperature | 1300 °F (704 °C) |
| Workpieces | Thread ring gage blocks, 1″ to 8 1/2″ diameter, 1/4″ to 1″ thick |
| Material | O6 oil-hardened steel |
| Hardness change | Rc 59-61 to Rc 45 in two zones, from the hole to the outside surface |
| Cycle time | 7.5 to 12 seconds depending on part size |
| Production rate | 250 to 300 parts per month |
The published reference data for the related bolt-shaft annealing application, which uses the same workhead architecture, is set out below as a comparison point for workhead and coil selection.
| Parameter | Value |
|---|---|
| Power supply | DW-UHF-4.5 kW induction heating system |
| Workhead | Remote workhead with one 0.66 µF capacitor |
| Induction coil | Custom-designed three-turn helical coil |
| Operating frequency | 280 kHz |
| Workpieces | Bolt shafts, various sizes |
| Materials | 431 stainless steel, Inconel, 8740 alloy steel |
| Target temperature, 431 stainless | 1850 °F (1010 °C) |
| Target temperature, Inconel and 8740 | 1000 °F (538 °C) |
| Cycle time, large bolts | 10–12 s |
| Cycle time, smaller bolts | 18–20 s |
| Coil changeover between sizes | None — the same coil is used |
For the wider equipment range, HLQ’s ultrahigh frequency induction heating series covers the full band, and the published method for this class of heat treatment is set out under why use induction annealing.